Jensen’s highest strength crown and bridge alloy, Jensen JYE Dental Noble Alloy is a versatile and economical Type 4 alloy. Dentists love the rich yellow color, technicians love the way JYE casts, finishes and polishes with ease and accuracy.
Features of Jensen JYE Dental Noble Alloy
Category: Crown & Bridge
Nobility: Noble
Color: Yellow
Composition: 52% Au, 5% Pd, 24% Ag
Ideal for: Demanding cases and everyday work
SPRUING The indirect method is recommended for multi-units. Use an 8 gauge runner bar with
10 gauge connectors. If preferred, the direct method may be used on both single units
and small bridges. Use a 10 gauge sprue 1/4” (6mm) to 3/8” (9mm) long. Sprues
longer than 3/8” (9mm) should have a reservoir 1/16” (1.5mm) from pattern. Patterns
should be a maximum of 1/4” (6mm) from top of investment.
INVESTMENT AND Either gypsum or phosphate bonded investment may used following the
BURNOUT manufacturer’s instructions. The burnout temperature should be at least 900ºF
(480ºC) and should not exceed 1200ºF (650ºC).
MELTING AND Extra winds of the casting arm are not required. A gas/compressed air or gas/oxygen
CASTING flame with 5 psi gas and 10 psi oxygen is recommended. The alloy will fully puddle
and form a ball before it is ready to cast. DO NOT OVERHEAT. The casting
temperature is 1750ºF (950ºC). Bench cool to obtain the hardened condition. Water
quench from a dull red heat to obtain the softened condition.
DEVESTING AND Blast with aluminum oxide to remove investment particles and oxidation. Finish and
FINISHING polish using standard techniques.